Home  About misconduct   中文  
 
  • Search
  • lucene Search
  • Citation
  • Fig/Tab
  • Adv Search
Just Accepted  |  Current Issue  |  Archive  |  Featured Articles  |  Most Read  |  Most Download  |  Most Cited

Chinese Journal of Stomatological Research(Electronic Edition) ›› 2012, Vol. 6 ›› Issue (03): 266-271. doi: 10.3877/cma.j.issn.1674-1366.2012.03.008

• Original Articles • Previous Articles    

Effect of hydroxyapatite coated porous NiTi alloy on hemolysis and cellular adhesion properties

Xin-ying SHI1, Tian TIAN1, Xue-li MAO1, Jing-xian ZHANG1, Xin-ping ZHANG,1(), Ke ZHAO1,()   

  1. 1.Guanghua School of Stomatology, Hospital of Stomatology, Sun Yat-sen University, Guangdong Provincial Key Laboratory of Stomatology, Guangzhou 510055, China
  • Received:2010-04-18 Online:2012-06-01 Published:2025-02-20
  • Contact: Xin-ping ZHANG, Ke ZHAO

Abstract:

Objective

To investigate the biocompatibility of the HA coated porous NiTi alloys in vitro. Hemolysis rate, cell attachment, proliferation, and ALP activity of the human fetal osteoblastic 1.19 cell line (hFOB 1.19) cultured on the HA coated porous NiTi alloys were measured.

Methods

A series of biocompatibility tests of porous NiTi alloy disc-shaped samples (10 mm in diameter and 2 mm in thickness) coated with HA were performed, and the untreated porous NiTi alloy and pure titanium samples were used for a comparative study. The hemolysis of all samples was tested by spectrophotometry.Scanning electron microscope (SEM) was used to observe morphology of hFOB 1.19 incubating on the samples, and MTS method and ALP kit were used to test cell attachment, proliferation and ALP activity.Repeated measurements were carried out with analysis of variance on the data.

Results

Hemolysis rates of the untreated NiTi alloy, HA-coated porous NiTi alloy and pure titanium samples are (0.30 ± 0.11)%,(0.51 ± 0.07)% and (0.27 ± 0.06)%, respectively, which are lower than 5% and acceptable according to the YY/T0127.1 standard. The SEM observation revealed that the hFOB 1.19 attached and spread well on the HA-coated porous NiTi alloy. The cell attachment and cell proliferation tests results showed that cells were better attached (P=0.000) and proliferated (P=0.001) on the HA-coated NiTi alloy samples than on the untreated NiTi alloy samples. ALP activity experimental results showed no significant difference between the HA-coated and untreated NiTi sample groups (P=1), but the samples in both groups exhibited higher ALP activity than the pure titanium samples (P=0.001, P=0.0004),respectively.

Conclusions

The results indicated that the HA-coated NiTi alloy and untreated NiTi alloy samples showed no hemolysis effect; HA coating can enhance the attachment and proliferation of hFOB 1.19 on the porous NiTi alloy, and ALP activity of the HA-coated and untreated porous NiTi alloys was higher than that of pure Ti.

Key words: Porous NiTi alloy, Surface coating, Hydroxyapatite, Hemocompatibility, Biocompatibility