中华口腔医学研究杂志(电子版) ›› 2025, Vol. 19 ›› Issue (02) : 132 -138. doi: 10.3877/cma.j.issn.1674-1366.2025.02.008

综述

牙科修复用可切削树脂渗透陶瓷关键性能及应用的研究进展
胡雨欣1, 吕广超1, 马骁1, 曹姗姗1, 李秋兰2, 赵克2, 张新平1,()   
  1. 1. 华南理工大学材料科学与工程学院,广州 510640
    2. 中山大学附属口腔医院,光华口腔医学院,广东省口腔医学重点实验室,广东省口腔疾病临床医学研究中心,广州 510055
  • 收稿日期:2024-12-03 出版日期:2025-04-01
  • 通信作者: 张新平
  • 基金资助:
    国家重点研发计划(2022YFC2410100)

Research advancement of the key properties and applications of machinable polymer-infiltrated-ceramicnetwork(PICN)composites for dental restorations

Yuxin Hu1, Guangchao Lyu1, Xiao Ma1, Shanshan Cao1, Qiulan Li2, Ke Zhao2, Xinping Zhang1,()   

  1. 1. School of Materials Science and Engineering,South China University of Technology,Guangzhou 510640,China
    2. Hospital of Stomatology,Guanghua School of Stomatology,Sun Yat-sen University,Guangdong Provincial Key Laboratory of Stomatology,Guangdong Provincial Clinical Research Center of Oral Diseases,Guangzhou 510055,China
  • Received:2024-12-03 Published:2025-04-01
  • Corresponding author: Xinping Zhang
引用本文:

胡雨欣, 吕广超, 马骁, 曹姗姗, 李秋兰, 赵克, 张新平. 牙科修复用可切削树脂渗透陶瓷关键性能及应用的研究进展[J/OL]. 中华口腔医学研究杂志(电子版), 2025, 19(02): 132-138.

Yuxin Hu, Guangchao Lyu, Xiao Ma, Shanshan Cao, Qiulan Li, Ke Zhao, Xinping Zhang. Research advancement of the key properties and applications of machinable polymer-infiltrated-ceramicnetwork(PICN)composites for dental restorations[J/OL]. Chinese Journal of Stomatological Research(Electronic Edition), 2025, 19(02): 132-138.

树脂渗透陶瓷(PICN)复合材料具有陶瓷的近天然牙特性和良好美学性能,以及树脂的易加工性等优点成为广受重视的牙科修复材料。本文综述了PICN的关键性能如力学性能、美学性能、生物相容性和粘接性能,以及各性能在不同使用环境下变化的研究现状,并对未来发展趋势进行了展望,旨在为研发人员进一步优化材料设计以改进性能提供参考,并为牙科医师临床应用时根据患者个人需求和实际应用场景合理选择与使用PICN材料提供依据。

Polymer-infiltrated-ceramic-network(PICN)composites have been given increasing attention as dental restorative materials due to the excellent combination of the mechanical compatibility with natural teeth,the lifelike aesthetic property stemmed from ceramics and the good machinability ascribed to the resin.This article presents a stateof-the -art review on PICN composites regarding their key properties,such as mechanical properties,aesthetic properties,biocompatibility and adhesive properties,as well as the changes of the above properties under different environment conditions,and finally provides an outlook for their future development trend.The main purpose of this article was to provide valuable instructions for researchers to further optimize the design of material properties,and also to offer a basis for dentists to reasonably select and use PICN composites according to patients′ personal preferences and practical use scenarios in clinical applications.

[1]
Eldafrawy M,Nguyen JF,Mainjot AK,et al.A functionally graded PICN material for biomimetic CAD-CAM blocks[J].J Dent Res,2018,97(12):1324-1330.DOI:10.1177/002203451 8785364.
[2]
Bona AD,Corazza PH,Zhang Y.Characterization of a polymerinfiltrated ceramic-network material[J].Dent Mater,2014,30(5):564-569.DOI:10.1016/j.dental.2014.02.019.
[3]
Coldea A,Swain MV,Thiel N. In vitro strength degradation of dental ceramics and novel PICN material by sharp indentation[J].J Mech Behav Biomed Mater,2013,26:34-42.DOI:10.1016/j.jmbbm.2013.05.004.
[4]
Hodásová L,Morena AG,Tzanov T,et al.3D-printed polymerinfiltrated ceramic network with antibacterial biobased silver nanoparticles[J].ACS Appl Bio Mater,2022,5(10):4803-4813.DOI:10.1021/acsabm.2c00509.
[5]
何三纲.口腔解剖生理学[M].8 版.北京:人民卫生出版社,2020:244-245.
[6]
Goujat A,Abouelleil H,Colon P,et al.Mechanical properties and internal fit of 4 CAD-CAM block materials[J].J Prosthet Dent,2018,119(3):384-389.DOI:10.1016/j.prosdent.2017.03.001.
[7]
Argyrou R,Thompson GA,Cho SH,et al.Edge chipping resistance and flexural strength of polymer infiltrated ceramic network and resin nanoceramic restorative materials [J].J Prosthet Dent,2016,116(3):397-403.DOI:10.1016/j.prosdent.2016.02.014.
[8]
郑梓婷,闫文娟.椅旁CAD/CAM 可切削材料相关性能的研究进展[J].口腔材料器械杂志,2019,28(3):46-51.DOI:10.11752/j.kqcl.2019.03.09.
[9]
孙瑞瞳,李享宜,胡一淳,等.硅基陶瓷的临床应用现状与展望[J/OL].中华口腔医学研究杂志(电子版),2021,15(2):72-78.DOI:10.3877/cma.j.issn.1674-1366.2021.02.002.
[10]
Ikemoto S,Nagamatsu Y,Masaki C,et al.Development of zirconia-based polymer-infiltrated ceramic network for dental restorative material[J].J Mech Behav Biomed Mater,2024,150:106320.DOI:10.1016/j.jmbbm.2023.106320.
[11]
Li WY,Sun J.Effects of ceramic density and sintering temperature on the mechanical properties of a novel polymerinfiltrated ceramic-network zirconia dental restorative(filling)material[J].Med Sci Monitor,2018,24:3068-3076.DOI:10.12659/MSM.907097.
[12]
Ikeda H,Nagamatsu Y,Shimizu H.Preparation of silica-poly(methyl methacrylate)composite with a nanoscale dual-network structure and hardness comparable to human enamel[J].Dent Mater,2019,35(6):893-899.DOI:10.1016/j.dental.2019.03.006.
[13]
Maryamnegari SM,Nateghi MR,Mohebat R.Effect of sintering and infiltration conditions on nanoscale dual network SiO2/polymethyl metacrylate composites mimicking human enamel[J].J Dent,2022,126:104311.DOI:10.1016/j.jdent.2022.104311.
[14]
胡雨欣,吕广超,马骁,等.牙科树脂渗透陶瓷复合材料制备的研究进展[J].国际口腔医学杂志,2025,52(1):133-140.DOI:10.7518/gjkq.2025012.
[15]
Peskersoy C,Sahan HM.Finite element analysis and nanomechanical properties of composite and ceramic dental onlays[J].Comput Methods Biomech Biomed Engin,2022,25(14):1649-1661.DOI:10.1080/10255842.2022.2032004.
[16]
Jansen JU,Lümkemann N,Sener B,et al.Comparison of fracture toughness measurements for zirconia materials using two test methods[J].Dent Mater J,2019,38(5):806-812.DOI:10.4012/dmj.2018-361.
[17]
Maleki M,Sheikh-Al-Eslamian SM,Hasani E,et al.Comparative study on the microstructure and mechanical behavior of monolithic ceramic and laminated composite of high strength 3YTZP and high fracture toughness 12Ce-TZP[J].J Alloy Compd,2019,776:166-171.DOI:10.1016/j.jallcom.2018.10.255.
[18]
Zang ST,He NX,Sun XT,et al.Influence of additives on the purity of tetragonal phase and grain size of ceria - stabilized tetragonal zirconia polycrystals(Ce-TZP)[J].Ceram Int,2019,45:394-400.DOI:10.1016/j.ceramint.2018.09.179.
[19]
Shahmiri R,Standard OC,Hart JN,et al.Optical properties of zirconia ceramics for esthetic dental restorations:A systematic review[J].J Prosthet Dent,2018,119(1):36-46.DOI:10.1016/j.prosdent.2017.07.009.
[20]
Mohammed NY,Wahsh MM,Motawea IT,et al.Fabrication and characterization of polymer-infiltrated ceramic network materials based on nano-tetragonal zirconia[J].J Korean Ceram Soc,2021,58:359-372.DOI:10.1007/s43207-020-00102-4.
[21]
Zhawi HE,Kaizer MR,Chughtai A,et al.Polymer infiltrated ceramic network structures for resistance to fatigue fracture and wear[J].Dent Mater,2016,32(11):1352-1361.DOI:10.1016/j.dental.2016.08.216.
[22]
Oudkerk J,Sanchez C,Grenade C,et al.The One-step No-prep technique for non-invasive full-mouth rehabilitation of worn dentition using PICN CAD-CAM restorations:Up to 9-year results from a prospective and retrospective clinical study[J].Dent Mater,2025,41(4):414-424.DOI:10.1016/j.dental.2024.12.016.
[23]
Song XF,Kang N,Yin L.Effect of bur selection on machining damage mechanisms of polymer infiltrated ceramic network material for CAD/CAM dental restorations[J].Ceram Int,2020,46(14):23116-23126.DOI:10.1016/j.ceramint.2020.06.089.
[24]
Tokunaga J,Ikeda H,Nagamatsu Y,et al.Castable polymerinfiltrated ceramic network composite for training model tooth with compatible machinability to human enamel[J].Dent Mater J,2022,41(4):520-526.DOI:10.4012/dmj.2021-299.
[25]
Tokunaga J,Ikeda H,Nagamatsu Y,et al.Wear of polymerinfiltrated ceramic network materials against enamel [J].Materials,2022,15(7):1-13.DOI:10.3390/ma15072435.
[26]
Alves MFRP,de Campos LQB,Simba BG,et al.Microstructural characteristics of 3Y - TZP ceramics and their effects on the flexural strength[J].Ceramics,2022,5(4):798-813.DOI:10.3390/ceramics5040058.
[27]
Wille S,Möller R,Kern M.Influence of shading on zirconia′s phase transformation and flexural strength after artificial aging[J].Dent Mater,2023,39(8):702-707.DOI:10.1016/j.dental.2023.06.005.
[28]
Gautam C,Joyner J,Gautam A,et al.Zirconia based dental ceramics:Structure,mechanical properties,biocompatibility and applications[J].Dalton T,2016,45(48):19194-19215.DOI:10.1039/c6dt03484e.
[29]
Li K,Kou HM,Rao JC,et al.Fabrication of enamel-like structure on polymer-infiltrated zirconia ceramics[J].Dent Mater,2021,37(4):e245-e255.DOI:10.1016/j.dental.2021.01.002.
[30]
Shirani M,Savabi O,Mosharraf R,et al.Comparison of translucency and opalescence among different dental monolithic ceramics[J].J Prosthet Dent,2021,126(3):446.e1-446.e6.DOI:10.1016/j.prosdent.2021.04.030.
[31]
Ruiz-López J,Espinar C,Lucena C,et al.Effect of thickness on color and translucency of a multi-color polymer-infiltrated ceramicnetwork material[J].J Esthet Restor Dent,2023,35(2):381-389.DOI:10.1111/jerd.12952.
[32]
Emamia N,Sjödahl M,Söderholm KM.How filler properties,filler fraction,sample thickness and light source affect light attenuation in particulate filled resin composites [J].Dent Mater,2005,21(8):721-730.DOI:10.1016/j.dental.2005.01.002.
[33]
Pulgar R,Lucena C,Espinar C,et al.Optical and colorimetric evaluation of a multi-color polymer-infiltrated ceramic-network material[J].Dent Mater,2019,35(7):e131-e139.DOI:10.1016/j.dental.2019.03.010.
[34]
Amri MD,Labban N,Alhijji S,et al. In vitro evaluation of translucency and color stability of CAD/CAM polymer-infiltrated ceramic materials after accelerated aging[J].J Prosthodont,2021,30(4):318-328.DOI:10.1111/jopr.13239.
[35]
Sulaiman TA,Suliman AA,Mohamed EA,et al.Optical properties of bisacryl-,composite-,ceramic- resin restorative materials:An aging simulation study[J].J Esthet Restor Dent,2021,33(6):913-918.DOI:10.1111/jerd.12653.
[36]
Acar O,Yilmaz B,Altintas SH,et al.Color stainability of CAD/CAM and nanocomposite resin materials[J].J Prosthet Dent,2016,115(1):71-75.DOI:10.1016/j.prosdent.2015.06.014.
[37]
Dos Santos DM,da Silva EVF,Watanabe D,et al.Effect of different acidic solutions on the optical behavior of lithium disilicate ceramics[J].J Prosthet,2017,118(3):430-436.DOI:10.1016/j.prosdent.2016.10.023.
[38]
Sen N,Us YO.Mechanical and optical properties of monolithic CAD-CAM restorative materials[J].J Prosthet Dent,2018,119(4):593-599.DOI:10.1016/j.prosdent.2017.06.012.
[39]
Lee JH,Kim SH,Yoon HI,et al.Colour stability and surface properties of high-translucency restorative materials for digital dentistry after simulated oral rinsing[J].Eur J Oral Sci,2020,128(2):170-180.DOI:10.1111/eos.12676.
[40]
Kilinc H,Turgut S.Optical behaviors of esthetic CAD-CAM restorations after different surface finishing and polishing procedures and UV aging:An in vitro study[J].J Prosthet Dent,2018,120(1):107-113.DOI:10.1016/j.prosdent.2017.09.019.
[41]
Choi YS,Kang KH,Att W.Evaluation of the response of esthetic restorative materials to ultraviolet aging[J].J Prosthet Dent,2021,126(5):679-685.DOI:10.1016/j.prosdent.2020.09.007.
[42]
Tassin M,Bonte E,Loison-Robert LS,et al.Effects of hightemperature - pressure polymerized resin - infiltrated ceramic networks on oral stem cells[J].Plos One,2016,11(5):e0155450.DOI:10.1371/journal.pone.0155450.
[43]
Pomès B,Behin P,Jordan L,et al.Influence of polymerization pressure and post - cure treatment on conversion degree and viscoelastic properties of polymer infiltrated ceramic network[J].J Mech Behav of Biomed,2021,115:104286.DOI:10.1016/j.jmbbm.2020.104286.
[44]
Puspitasari R,Irnawati D,Widjijono.The effect of zinc oxide(ZnO)nanoparticle concentration on the adhesion of mucin and streptococcus mutans to heat-cured acrylic resin[J].Dent Mater J,2023,42(6):791-799.DOI:10.4012/dmj.2023-016.
[45]
Tang FL,Li JL,Xie WH,et al.Bioactive glass promotes the barrier functional behaviors of keratinocytes and improves the Reepithelialization in wound healing in diabetic rats[J].Bioact Mater,2021,6(10):3496-3506.DOI:10.1016/j.bioactmat.2021.02.041.
[46]
Chen YY,Sun C,Cao JF,et al.Mechanical properties and in vitro biocompatibility of hybrid polymer-HA/BAG ceramic dental materials[J].Polymers,2022,14(18):3774.DOI:10.3390/polym14183774.
[47]
Cui BC,Zhang RR,Sun FB,et al.Mechanical and biocompatible properties of polymer-infiltrated-ceramic-network materials for dental restoration[J].J Adv Ceram,2020,9(1):123-128.DOI:10.1007/s40145-019-0341-5.
[48]
Sismanoglu S,Gurcan AT,Yildirim-Bilmez Z,et al.Mechanical properties and repair bond strength of polymer-based CAD/CAM restorative materials[J].Int J Appl Ceram Technol,2021,18:312-318.DOI:10.1111/ijac.13653.
[49]
Yano HT,Ikeda H,Nagamatsu Y,et al.Effects of alumina airborne-particle abrasion on the surface properties of CAD/CAM composites and bond strength to resin cement[J].Dent Mater J,2021,40(2):431-438.DOI:10.4012/dmj.2020-023.
[50]
Wanderico CM,Picolo MZ,Kury M,et al.Alternative surface treatments strategies for bonding to CAD/CAM resin - matrix ceramics[J].J Adhes Sci Technol,2022,37(8):1471-1484.DOI:10.1080/01694243.2022.2079333.
[51]
Tuncer B,Aktas G,Baris Guncu M,et al.Effects of surface treatments and cement type on shear bond strength between titanium alloy and All-Ceramic materials[J].Materials,2023,16(18):86240.DOI:10.3390/ma16186240.
[52]
Eldafrawy M,Greimers L,Bekaert S,et al.Silane influence on bonding to CAD - CAM composites:An interfacial fracture toughness study[J].Dent Mater,2019,35(9):1279-1290.DOI:10.1016/j.dental.2019.05.019.
[53]
Komagata Y,Nagamatsu Y,Ikeda H.Comparative bonding analysis of computer-aided design/computer-aided manufacturing dental resin Composites with various resin cements[J].J Compos Sci,2023,7(10):1-11.DOI:10.3390/jcs7100418.
[54]
Bello YD,Di Domenico MB,Magro LD,et al.Bond strength between composite repair and polymer - infiltrated ceramic -network material:Effect of different surface treatments[J].J Esthet Restor Dent,2019,31(3):275-279.DOI:10.1111/jerd.12445.
[55]
王淑君,张楚晗,唐一阳,等.自粘接树脂水门汀的临床应用及展望[J/OL].中华口腔医学研究杂志(电子版),2024,18(4):276-286.DOI:10.3877/cma.j.issn.1674-1366.2024.04.010.
[56]
David-Pérez M,Ramírez-Suárez JP,Latorre-Correa F,et al.Degree of conversion of resin-cements(light-cured/dual-cured)under different thicknesses of vitreous ceramics:Systematic review[J].J Prosthodont Res,2022,66(3):385-394.DOI:10.2186/jpr.JPR_D_20_00090.
[57]
Spitznagel FA,Röhrig S,Langner R,et al.Failure load and fatigue behavior of monolithic translucent zirconia,PICN and rapid-layer posterior single crowns on zirconia implants[J].Matrials(Basel),2021,14(8):1990.DOI:10.3390/ma14081990.
[58]
Rosentritt M,Krifka S,Preis V,et al.Dynamic fatigue of composite CAD/CAM materials[J].J Mech Behav Biomed,2019,98:311-316.DOI:10.1016/j.jmbbm.2019.07.002.
[59]
Coldea A,Fischer J,Swain MV,et al.Damage tolerance of indirect restorative materials(including PICN)after simulated bur adjustments[J].Dent Mater,2015,31(6):684-694.DOI:10.1016/j.dental.2015.03.007.
[60]
Elraggal A,Afifi RR,Alamoush RA,et al.Effect of acidic media on flexural strength and fatigue of CAD - CAM dental materials[J].Dent Mater,2023,39(1):57-69.DOI:10.1016/j.dental.2022.11.019.
[61]
Turker I,Kursoglu P.Effects of thermal ageing on the mechanical properties of cad-cam ceramic materials[J].Ceramcs-Silikáty,2023,67(4):496-504.DOI:10.13168/cs.2023.0049.
[62]
Turgut S,Kılınç H,Bağış B.Effect of UV aging on translucency of currently used esthetic CAD-CAM materials[J].J Esthet Restor Dent,2019,31(2):147-152.DOI:10.1111/jerd.12460.
[1] 李帝均, 王斌. 肩袖损伤修复的生物材料选择及动物模型评价[J/OL]. 中华关节外科杂志(电子版), 2024, 18(01): 118-124.
[2] 柴浩卜, 王俏杰, 张先龙. 具有骨免疫调节性能的骨科生物材料研究进展[J/OL]. 中华关节外科杂志(电子版), 2022, 16(01): 37-43.
[3] 于承浩, 张益, 陈进利, 戚超, 李海峰, 于腾波. 肩袖补片在巨大肩袖损伤治疗中的研究进展[J/OL]. 中华关节外科杂志(电子版), 2021, 15(02): 225-230.
[4] 黄弘轩, 白波, 赖琛, 王瑛, 陈艺, 张姝江. 高分子修饰细菌纤维素细胞相容性的初步研究[J/OL]. 中华关节外科杂志(电子版), 2020, 14(01): 63-67.
[5] 张廷帅, 邹健宇, 陈汉政, 刘日许, 郑仕聪, 陈艺, 张姝江, 姚咏嫦. 三维共培养体系促进去分化的软骨细胞再分化的实验研究[J/OL]. 中华关节外科杂志(电子版), 2019, 13(06): 693-698.
[6] 贾古友, 刘树民, 王晗, 唐绪军, 王晓光, 刘震, 胡永成. 抗菌涂层改性预防骨科内植物感染生物膜形成的研究进展[J/OL]. 中华关节外科杂志(电子版), 2018, 12(04): 544-550.
[7] 王晟, 许卓然, 夏德萌, 李磊, 许硕贵. 穿皮骨整合截肢假体与上皮细胞生长迁移的研究进展[J/OL]. 中华损伤与修复杂志(电子版), 2021, 16(02): 166-169.
[8] 李琳, 杨文, 王晓东. 树脂陶瓷复合材料的研究及临床应用现状[J/OL]. 中华口腔医学研究杂志(电子版), 2024, 18(02): 80-88.
[9] 张楚晗, 王淑君, 韦孟廷, 蒋欣怡, 苏冠宇, 战德松, 付佳乐. 玻璃离子水门汀的临床应用与展望[J/OL]. 中华口腔医学研究杂志(电子版), 2023, 17(04): 299-308.
[10] 黄石头, 魏洪波, 李德华. 三维打印钛种植体性能及临床应用的研究进展[J/OL]. 中华口腔医学研究杂志(电子版), 2023, 17(01): 1-9.
[11] 孙瑞瞳, 李享宜, 胡一淳, 高嘉阳, 胡博, 战德松, 付佳乐. 硅基陶瓷的临床应用现状与展望[J/OL]. 中华口腔医学研究杂志(电子版), 2021, 15(02): 72-78.
[12] 郭丽娜, 王晓东, 张新平, 简裕涛, 赵克. 代型材料力学性能对磨牙氧化锆全瓷冠断裂失效行为的影响[J/OL]. 中华口腔医学研究杂志(电子版), 2019, 13(01): 7-12.
[13] 于茜, 周建辉, 赵小淋, 谢大洋, 曹雪莹. 血液净化膜材料的临床发展[J/OL]. 中华肾病研究电子杂志, 2021, 10(02): 103-108.
[14] 谭亚运, 张民. 硅酸盐/磷酸盐复合型骨水泥的研究现状及新进展[J/OL]. 中华临床医师杂志(电子版), 2017, 11(13): 1993-1996.
[15] 张帅, 刘凯, 王刚刚, 倪才方, 陈珑. 不同降温法延长椎体成形术中骨水泥注射时间的骨水泥材料性能研究[J/OL]. 中华介入放射学电子杂志, 2024, 12(03): 228-233.
阅读次数
全文


摘要